Tie-Layer MFR Explained: 2.3 vs 70 g/10 min in Bondine and Orevac Grades
A converter once rejected a tie-layer resin after a two-week trial and called it "the same material with a different bag". The two grades really were in the same adhesive family, and both were maleic-anhydride functionalised. What differed was the melt flow rate: one was around 3 g/10 min, the other around 70. On a cast coextrusion line the high-flow grade dispersed easily but could not hold the layer shape at the die; on a hot-melt route the low-flow grade never reached a workable viscosity.
MFR is the first number that separates tie-layer grades, but it is not an adhesion rating. This guide uses the published data for the seven tie-layer grades currently listed on our site, so you can see what each number actually means in selection terms.
Contents
- What MFR actually measures
- Seven tie-layer grades side by side
- The three flow bands and what they are for
- Why the base resin matters as much as flow
- Three common selection mistakes
- What to put in a tie-layer RFQ
- FAQ
What MFR Actually Measures
Melt flow rate (also called MFI) is the mass of polymer extruded through a standard die in ten minutes under a stated temperature and load. The test method is ASTM D1238. Most of the tie-layer grades below publish their flow at 190 °C / 2.16 kg — always quote the condition with the number, because the same resin measured under a different load gives a different figure.
For a tie layer, flow tells you two things: how easily the resin melts and disperses in the extruder, and roughly how much melt strength the layer will have at the die. Those pull in opposite directions. Higher MFR generally means easier processing and lower melt strength; lower MFR means a stiffer melt that holds shape better but asks more of the equipment.
Reading a TDS and COA explains why these figures are typical values, not guaranteed specifications.
Seven Tie-Layer Grades Side by Side
All figures below are the published values on the individual product pages of this site. No value is estimated or inferred.
| Grade | Base / family | MFR (g/10 min) | Density (g/cm³) | Melting point | Vicat |
|---|---|---|---|---|---|
| HX8290 | Bondine, E-EA-MAH | 70 | 0.94 | 85 °C | 40 °C |
| LX4110 | Bondine, EEA-MAH | 5 | 0.94 | 105 °C | 78 °C |
| 18211 | Orevac, EVA-g-MAH | 3.5 | 0.95 | 75 °C | 51 °C |
| 18215 | Orevac, EVA-g-MAH | 4 | 0.95 | 75 °C | — |
| 18342N | Orevac, HDPE-g-MAH | 3.5 | 0.93 | 125 °C | 110 °C |
| OE850 | Orevac, LDPE-g-MAH | 7.5 | 0.91 | 104 °C | 89 °C |
| 18300 | Orevac, LLDPE-g-MAH | 2.3 | 0.91 | 120 °C | 85 °C |
Typical published values. Where the source data does not state a figure, the cell is left blank rather than filled with an estimate. Confirm the current TDS and batch COA before ordering.
The Three Flow Bands and What They Are For
High flow: HX8290 at 70 g/10 min
HX8290 is in a different flow class from everything else in this set. At 70 g/10 min, 85 °C melting and Vicat 40 °C, it is a low-heat, easy-dispersion grade. The product page lists hot-melt adhesive and lamination/compounding among its routes — applications where getting the adhesive to flow and wet the surface dominates. It is not the grade to pick for a high-temperature coextruded layer simply because it is "the same Bondine family" as LX4110.
Mid flow: OE850 at 7.5 and LX4110 at 5 g/10 min
These two sit in the useful middle. OE850 (LDPE-g-MAH, 0.91 g/cm³, melting 104 °C, Vicat 89 °C) combines moderate heat resistance with easier flow. LX4110 (EEA-MAH, melting 105 °C, Vicat 78 °C) is described in its source data as thermally stable. When a structure needs a balance between processability and heat resistance, this is the band to start from.
Low flow: 18211 / 18215 / 18342N / 18300 at 2.3–4 g/10 min
The low-flow group splits by base resin rather than by flow. 18211 and 18215 are EVA-backed and melt at 75 °C — the low-temperature option. 18342N (HDPE-g-MAH, melting 125 °C, Vicat 110 °C) and 18300 (LLDPE-g-MAH, melting 120 °C, Vicat 85 °C) are the high-heat options, with 18342N carrying the highest Vicat figure in this set. Their flow rates are close, but the temperature window is not.
For a structured introduction to the families, see Tie-Layer Compound Selection: PE-g-MAH vs PP-g-MAH vs EAA and Bondine vs Bynel vs Primacor vs Igetabond.
Why the Base Resin Matters as Much as Flow
A tie layer has to bond to both sides of a multilayer structure. The MAH functionality is what makes the bond possible; the base resin determines whether the layer is compatible with the neighbouring PE, PP, EVA or barrier layer and what temperature it can survive.
- EVA-g-MAH (18211, 18215) — lowest melting point in this set, around 75 °C. Useful where the adjacent layers cannot take high temperature.
- LDPE-g-MAH (OE850) — lowest density (0.91 g/cm³) with a mid-range melting point.
- LLDPE-g-MAH (18300) — same density band as OE850 but a melting point of 120 °C and the lowest flow here.
- HDPE-g-MAH (18342N) — highest melting point and Vicat, suited to the hottest coextrusion structures.
- Bondine E-EA-MAH / EEA-MAH (HX8290, LX4110) — adhesive-focused families where the acrylate content, rather than the PE backbone, drives the balance.
Matching the base resin to the structure comes before comparing MFR. A grade with the perfect flow number but the wrong backbone will still delaminate. Our What Is a Tie-Layer Resin? explains the bonding mechanism in more detail.
Three Common Selection Mistakes
- Comparing flow numbers without the test condition. 190 °C / 2.16 kg is the condition quoted on most of these pages. A number measured under a different load is not directly comparable.
- Assuming higher MFR means better adhesion. Flow affects wetting and dispersion; adhesion depends on the functional chemistry and the surfaces being bonded. HX8290 at MFR 70 and 18300 at MFR 2.3 solve different problems.
- Ignoring the thermal end of the data sheet. Melting point and Vicat tell you whether the tie layer survives the downstream process. 18211 at 75 °C melting and 18342N at 125 °C are not interchangeable even though their MFR is the same.
What to Put in a Tie-Layer RFQ
To shortlist a grade quickly, send us:
- The full layer structure, from outside to inside, including the tie layer position.
- Which two materials the tie layer must bond.
- The conversion route (cast film, blown film, lamination, coating, compounding) and the melt temperature you can actually run.
- Any downstream heat step — retort, hot fill, sterilisation or heat sealing.
- Target MFR window, if your process team already has one.
- Required documents: TDS, SDS, batch COA, and any food-contact or compliance letter.
Browse all grades in the Tie-Layer & Compatibilizers category, or send an inquiry with the structure above.
FAQ
Which tie-layer grade has the highest MFR?
HX8290 at 70 g/10 min, based on the published data on this site. It is a hot-melt / lamination-oriented grade, not a high-temperature coextrusion tie layer.
Which grade has the highest heat resistance?
18342N (HDPE-g-MAH) has the highest published melting point (125 °C) and Vicat (110 °C) in this set.
Are 1601 and 1601-2 the same product?
They publish identical MFR, density, melting point and Vicat figures, but are described differently by ion type on their product pages. Always confirm the exact grade on the current TDS before substituting.
Can you substitute a tie-layer grade with the same MFR?
Only after checking the base resin and the layer structure. 18211 and 18342N both publish MFR 3.5, but melt at 75 °C and 125 °C respectively.
References
- ASTM D1238, Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Plastometer.
- Individual grade data published on the POLYVALA product pages linked in the table above.
- How to Read a TDS and COA and EVOH Barrier Resin Selection Guide.
Next Step
Send us your layer structure and process conditions, and we will shortlist two or three grades from the seven above with the published figures attached. Start an inquiry.