EVOH Barrier Resin Selection Guide: Ethylene Content, Layer Structure and Processing

2026-11-12
EVOH Barrier Resin Selection Guide: Ethylene Content, Layer Structure and Processing

EVOH is the default answer when a package has to keep oxygen out for months. It is also the resin most often specified incorrectly: buyers pick a grade by a single OTR number, then discover that humidity, layer position, tie-layer choice and thermal history change the result more than the grade itself. This guide is a selection framework, not a datasheet — it walks through the decisions in the order they actually matter, and links to the grades and documents you need at each step. Start with our EVOH barrier resin range if you already know the structure you are running.

1. What EVOH Actually Does — and What It Cannot Do Alone

Ethylene vinyl alcohol copolymer is made by saponifying an ethylene-vinyl acetate copolymer. The vinyl alcohol groups pack tightly and create a polar, hydrogen-bonded structure that is exceptionally resistant to oxygen, nitrogen, carbon dioxide, aromas and many solvents. That is why a layer only a few micrometres thick can replace centimetres of a plain polyolefin.

The same chemistry creates the two limitations that shape every design decision. First, those hydroxyl groups are hydrophilic: EVOH picks up moisture, and a wet EVOH layer loses a significant part of its oxygen barrier. Second, EVOH is stiff and has poor adhesion to polyethylene and polypropylene on its own. In practice EVOH is never the outside layer and never used alone — it is a thin core inside a coextruded structure, protected by polyolefin skins and held in place by adhesive tie layers. If you are choosing between EVOH, PVDC and nylon for a specific shelf-life target, our explainer on ethylene content and OTR covers the trade-off in more detail.

2. Ethylene Content: The One Number That Sets Everything Else

Ethylene content (expressed in mol%) is the primary grade differentiator. Lower ethylene content means more vinyl alcohol groups per unit length: better oxygen barrier, higher crystallinity, a higher melting point, greater moisture sensitivity and a narrower processing window. Higher ethylene content softens the resin, widens the processing window and improves thermoformability, at the cost of barrier performance.

The four commercial steps most buyers encounter are 29, 32, 38 and 44 mol%. The melting points below are indicative values taken from the grades listed on this site — always confirm the exact figure on the official TDS before setting extruder zones.

Ethylene contentIndicative melting pointOxygen barrierProcessing behaviourTypical fit
29 mol%≈ 188 °CHighestNarrowest window, stiffest, most moisture-sensitiveHigh-barrier and retort structures
32 mol%≈ 183 °CVery highStandard coextrusion windowGeneral food packaging, barrier film
38 mol%≈ 173 °CHighWider window, easier thermoformingSheet, trays, bottles, deep-draw
44 mol%≈ 165 °CModerate (relative)Widest window, most flexibleCoextrusion coating, flexible structures

Notice what is missing: an OTR number. Oxygen transmission rate is measured at a stated temperature and relative humidity on a stated thickness, and quoting it without those conditions is meaningless. Compare grades at the same test conditions, on the same layer thickness, and at the humidity your package will actually see.

3. Humidity: The Reason EVOH Is Never the Outside Layer

Water molecules disrupt the hydrogen bonding that gives EVOH its barrier. Under high relative humidity, oxygen transmission rises — sometimes by a large multiple — and it recovers only as the resin dries out again. This is not a defect you can engineer away by picking a "better" grade; it is intrinsic to the chemistry.

The design response is structural. Keep the EVOH layer away from both the product side (which may be wet) and the ambient side (which may be humid), and give the polyolefin skins enough thickness to slow moisture ingress. In retort applications, where the package sees saturated steam, the effect is acute and temporary — see section 8. When a spec sheet promises a barrier figure without stating RH, treat it as a screening value only.

4. Where the EVOH Layer Goes in a Multilayer Structure

A barrier structure is a stack, and the position of each layer is a decision. The simplest workable arrangement is five layers; seven-layer lines add a nylon layer for toughness, a reclaim layer, or extra sealant bulk.

Layer5-layer example7-layer exampleJob
1 (outside)PE or PPPA / PPPrint surface, abrasion, moisture shield
2TieTieBond skin to core
3EVOHEVOHOxygen barrier (often only a few µm)
4TieTieBond core to sealant
5PE sealantPA or reclaimSeal integrity / toughness
6–7—Tie + PE sealantExtra barrier balance, heat seal

Two rules follow. The EVOH layer should be as thin as the barrier target allows — it is the most expensive and the most moisture-sensitive component. And the tie layers on both sides must be compatible with both neighbours, because delamination usually starts at the interface, not in the barrier layer.

5. Matching a Grade to the Job

Once the structure is fixed, grade selection becomes much simpler. The EVASIN series from Chang Chun Petrochemical (Taiwan, China) spans all four ethylene-content steps, so it is a useful single-family reference. For maximum barrier in a retort or long-shelf-life pack, start at the low-ethylene end: EVASIN EV2951F (29 mol%) is the reference point, with EV3251F (32 mol%) offering a slightly friendlier process window. Where thermoforming depth and line speed matter more than the last increment of barrier, EV3851F (38 mol%) and EV4405F (44 mol%) are the usual candidates.

It is worth shortlisting an equivalent from a second supplier family at the same time. Kuraray E105B, Kuraray F101B / F171B and Nippon Gohsei E3808 / ET3803RB are comparable options we list, and running two approved sources is cheaper insurance than a single-source qualification. Ask for samples from both before you freeze the BOM.

6. Tie Layers Are Half of the Decision

EVOH does not bond to PE or PP by itself. The adhesive layers are typically anhydride-grafted polyolefins or acid copolymers, and they have to survive the same thermal history as the barrier layer. A tie resin with too low a melt strength will thin out at the edges of a wide die; one with too high a viscosity can disturb layer uniformity.

This is why we treat tie-layer and compatibilizer grades as part of the same selection exercise. Grades such as SK BONDINE TX8030 are formulated for PA / EVOH / PE structures that see retort conditions, while EAA 3330 and the wider EAA / EMAA range cover adhesion to metal, paper and foil. Our guide to EAA and EMAA adhesive resins explains how acid content and melt index affect bond strength and hot tack.

7. Processing Window: Temperature, Residence Time, Purging

EVOH is processed in the same general temperature region as the surrounding polyolefin layers, which is what makes coextrusion possible. The exact zone profile belongs on the supplier's TDS, not in a general guide. What matters across all grades is thermal discipline: keep residence time short, avoid dead spots in the adapter and die, and purge with a polyolefin before any extended shutdown. Prolonged exposure to high temperature promotes degradation and gel formation, and gels in a barrier layer show up as pinholes in finished film.

Layer thickness control is the second discipline. Because the EVOH layer is thin, a small percentage variation in total output can move the barrier layer far enough to change OTR measurably. Ask your converter for a layer-distribution report on the first article, and re-check it after any die or throughput change. Moisture management matters too: keep resin sealed until use and follow the supplier's drying guidance rather than assuming EVOH behaves like polyethylene.

8. Retort and Hot-Fill: What Changes After 121 °C

Steam sterilisation drives moisture into the EVOH layer at exactly the moment the package needs its barrier most. Oxygen transmission rises during and immediately after the cycle, then falls as the structure dries — a recovery period that can matter for shelf-life modelling. Design responses include a slightly thicker barrier layer, higher-barrier low-ethylene grades, moisture-scavenging layers, and an asymmetric structure that puts the drier side toward the EVOH.

Do not qualify a retort structure on flat-film OTR data alone. Test the finished package after the actual sterilisation cycle and after a defined recovery interval, then compare peel strength at the tie interfaces as well. Retort is also where tie-layer selection is most likely to fail, so validate the whole stack rather than the barrier resin in isolation.

9. Documentation to Request Before You Place an Order

Four documents separate a smooth qualification from a costly one: the current TDS (grade-specific values and test conditions), a lot-specific COA, the SDS, and a food-contact compliance statement for your target market. If a number in a quotation does not appear on the TDS, ask where it came from. Our walkthrough of TDS and COA documents lists the six numbers worth verifying on every lot, and our data sources and TDS request policy explains how we compile and label the property data on this site.

For a new structure, also request a sample with a stated lot number, and record the layer distribution and retort cycle used in your trial. Those three records make a future supplier change auditable instead of anecdotal.

10. Building a Shortlist

A practical shortlist has two EVOH grades at different ethylene contents, two compatible tie resins, and a documented reason for each. Send us your structure (layer order and thicknesses), shelf-life target, filling or sterilisation cycle, and the OTR test conditions your customer uses. We will come back with grade options, sample availability and the current TDS for each — see the full EVOH range or contact the technical team directly.

The goal is not the highest barrier number on paper. It is a structure that holds its barrier at the humidity, temperature and handling your package actually sees, at a layer thickness your line can hold consistently.

About This Article

This guide is prepared by the POLYVALA technical team. All property values, test methods and compliance statements are drawn from manufacturer Technical Data Sheets (TDS) and recognized standards (ASTM, ISO). Figures must always be confirmed against the current official TDS and the lot-specific Certificate of Analysis (COA) before production qualification.

References

  • Manufacturer Technical Data Sheets (TDS) for the grades referenced above.
  • ASTM D1238 / ISO 1133 — Melt flow rate (MFR/MFR) of thermoplastics.
  • ASTM D1505 / ISO 1183 — Density of plastics by the density-gradient technique.
  • ASTM D638 — Tensile properties of plastics.

About this article

Written by the technical team at Shanghai Polyvala Plastics, a sourcing and compounding partner for specialty polymer buyers since 2013. We check grades against manufacturer TDS and lot-specific COA rather than marketing claims. Questions about a grade or an equivalent? Request the TDS and COA, or contact our application engineers for a line-specific recommendation.

Recommended

View all articles