Delamination Troubleshooting: When It Is Not the Tie Resin's Fault
A converter sees the layers peel apart in a retort pouch, replaces the tie resin, and the problem stays. The tie layer is the most visible suspect, so it gets changed first — but in a multilayer structure the bond can fail for reasons that have nothing to do with the adhesive grade. This guide walks through the checks that come before you change the tie resin, using the published data of the EVOH and tie-layer grades listed on our site.
The point is not to defend a particular product. It is to avoid paying for a grade change when the real cause is moisture, temperature, layer thickness, or a surface that was never clean.
Contents
- First: where exactly is the split?
- Cause 1 — moisture in the barrier layer
- Cause 2 — tie layer too thin or wrong flow
- Cause 3 — surface contamination and untreated film
- Cause 4 — thermal and melting-point mismatch
- Cause 5 — die and process conditions
- The grade data that matters
- What to send before asking for a new grade
- FAQ
First: Where Exactly Is the Split?
"Delamination" is a symptom, not a diagnosis. Before changing anything, peel a sample by hand and look at where the separation happens:
- Clean split between tie and barrier — points to adhesion, surface preparation, or tie-layer thickness.
- Barrier layer itself cracks or powders — points to moisture or to a layer that was run outside its thermal window.
- Split after retort but not before — points to thermal expansion mismatch or to moisture picked up during processing.
- Split at the seal area only — points to seal contamination or to tie resin being squeezed out at the seal jaws.
The location narrows the cause faster than any grade swap. What Is a Tie-Layer Resin explains what the tie layer is — and just as importantly, what it cannot do.
Cause 1 — Moisture in the Barrier Layer
EVOH is hygroscopic. If the barrier resin absorbs moisture before or during coextrusion, the water turns to steam at processing temperature, creating voids and weak boundaries that look exactly like poor adhesion. Changing the tie resin will not fix this.
The grades in our EVOH range illustrate why the barrier choice matters. Published melting points run from 164 °C (e.g. Nippon Gohsei A4412B / AT4403B, Wanhua EV-4415) to 190 °C (Kuraray L171B, Chang Chun EVASIN EV2951F), with density from 1.14 to 1.21 g/cm³. Higher-ethylene grades such as the 1.14 g/cm³ grades (EV4405F, E105B, EV-4415) are generally more forgiving on moisture than the 1.19–1.21 g/cm³ grades (EV3251F, F101B, EW-3201, EV-2935). If the line is running a high-barrier, low-ethylene grade and the film is seeing humidity before extrusion, drying and resin handling come first.
Ask for the drying condition on the COA and check the hopper residence time. How to Read a TDS and COA covers which fields actually tell you this.
Cause 2 — Tie Layer Too Thin or Wrong Flow
A tie layer has to be thick enough to form a continuous film and fluid enough to wet the substrate at the die temperature. Two published numbers tell you most of what you need: melt flow rate and melting point.
In our tie-layer range, the OREVAC® grades span MFR 2.3 to 7.5 g/10 min at 190 °C / 2.16 kg — for example 18300 at 2.3, 18211 and 18342N at 3.5, LX4110 (BONDINE®) at 5, and OE850 at 7.5. BONDINE® HX8290 sits much higher at 70 g/10 min under the same condition, with a Vicat of 40 °C. These are not interchangeable flow behaviours: a high-flow grade wets easily but holds less melt strength at the die, while a low-flow grade needs more pressure and heat to spread.
If the current tie layer is running at a thickness below the continuous-film threshold, increasing gauge often fixes delamination without any grade change. If the grade's melting point is far above the barrier layer's, it may not be fully molten where the bond is formed — see the next section.
For a deeper read on the flow numbers, see Tie-Layer MFR Explained and the brand comparison in Bondine vs Bynel vs Primacor vs Igetabond.
Cause 3 — Surface Contamination and Untreated Film
If the substrate surface is contaminated or under-treated, even the right tie resin will peel off cleanly. Typical culprits are residual solvent, silicone-based release agents, anti-block additives migrating to the surface, or a corona treatment level that has decayed before coextrusion.
Practical checks:
- Run a dyne test on the substrate immediately before the line, not from a coil stored for days.
- Check for a clean, uniform peel surface — a sticky or stringy failure usually means the tie layer itself is too weak, not the surface.
- If a primer or tie layer is applied to metal foil, confirm the foil surface is degreased and dry.
Cause 4 — Thermal and Melting-Point Mismatch
A multilayer bond forms only when both surfaces are molten at the interface. Compare melting points across the stack. In our published data:
- Tie grades: 75 °C (18211, 18215), 85 °C (HX8290), 104–105 °C (LX4110, OE850), 120 °C (18300), 125 °C (18342N).
- EVOH grades: 164–165 °C (EV4405F, E105B, EV-4415, A4412B), 172–173 °C (H171B, EV3851F, EW-3801), 183 °C (EV3251F, F101B, EW-3201), 188–190 °C (EV2951F, EW-2901, EV-2935, L171B).
A tie grade melting at 75 °C against an EVOH melting at 190 °C is not automatically wrong — the tie resin is not required to match the barrier's melting point — but the die and adapter temperatures must be high enough to bring both into a bondable state without degrading either. If the tie layer cools and skins over before contact with the barrier, the bond never forms. Check the temperature profile across the die, not just the barrel setpoints.
Cause 5 — Die and Process Conditions
Even with the correct grades, the layer can fail if the process starves it:
- Die lip alignment — a misaligned die puts the tie layer slightly off the intended interface.
- Melt fracture or surging — a high-viscosity tie grade running above its stable shear window produces a wavy, discontinuous layer.
- Quench and draw-down — rapid cooling or high draw ratio can lock in stress that opens as a delayed split days later.
- Post-processing — converting tension, slitting, and sealing conditions can all reveal a marginal bond.
The Grade Data That Matters
The table below uses only published values from the grades currently listed on this site. Where a field is not published, it is left blank rather than estimated.
| Grade | MFR (g/10 min) | Test condition | Density (g/cm³) | Melting point (°C) |
|---|---|---|---|---|
| OREVAC 18211 | 3.5 | 190 °C / 2.16 kg | 0.95 | 75 |
| OREVAC 18215 | 4 | — | 0.95 | 75 |
| OREVAC 18300 | 2.3 | 190 °C / 2.16 kg | 0.91 | 120 |
| OREVAC 18342N | 3.5 | 190 °C / 2.16 kg | 0.93 | 125 |
| OREVAC OE850 | 7.5 | 190 °C / 2.16 kg | 0.91 | 104 |
| BONDINE LX4110 | 5 | 190 °C / 2.16 kg | 0.94 | 105 |
| BONDINE HX8290 | 70 | 190 °C / 2.16 kg | 0.94 | 85 |
| EVASIN EV2951F (EVOH) | 3 | 210 °C / 2.16 kg | 1.20 | 188 |
| EVASIN EV3251F (EVOH) | 1.6 | 190 °C / 2.16 kg | 1.19 | 183 |
| EVASIN EV4405F (EVOH) | 5.5 | 190 °C / 2.16 kg | 1.14 | 165 |
Browse the full ranges: Tie-Layer & Compatibilizers and EVOH Barrier Resins.
What to Send Before Asking for a New Grade
If you have done the five checks above and still need a grade change, send this with your inquiry — it lets us suggest a grade that fits the line instead of guessing:
- Full layer structure with nominal thickness of each layer.
- Which interface actually splits, with a photo of the peeled surface.
- Extruder and die temperatures, line speed, and draw-down ratio.
- The tie grade and EVOH grade currently running, with their MFR test conditions.
- Whether the failure appears immediately or after retort / storage.
Send these through our inquiry form. We respond with grade options, TDS, and lead time — not with a generic sales reply.
FAQ
Does a higher-MFR tie resin always bond better?
No. Higher MFR improves wetting but reduces melt strength. The right flow depends on your die geometry, line speed, and the layer you are bonding to.
Can moisture in EVOH really look like tie-layer failure?
Yes. Absorbed moisture turns to steam at processing temperature and creates voids at the interface. The peeled surface looks like an adhesion failure, but the cause is resin handling.
Should the tie layer melting point match the EVOH grade?
Not necessarily. What matters is that both layers are bondable at the interface temperature. Compare the melting points in the table as a starting point, then check the die temperature profile.
Can I fix delamination by increasing tie-layer thickness?
If the current layer is below the continuous-film threshold, yes. If the surface is contaminated or the barrier is wet, extra thickness will not help.