EMA vs EBA Grade Map: LOTRYL and Exxtra Resins by MFR

EMA and EBA: Two Ethylene Copolymers That Get Confused

Buyers searching for a flexible, polar, easy-to-bond polyethylene often land on two names that look interchangeable: EMA (ethylene–methyl acrylate) and EBA (ethylene–butyl acrylate). Both are random copolymers of ethylene with an acrylate comonomer, both are softer and more polar than plain PE, and both are supplied in pellet form under families such as LOTRYL and Exxtra. But the comonomer is different, and that difference shows up in flexibility, heat resistance and the grades available at a given melt flow. This guide maps the EMA and EBA grades currently listed on our site using their published melt flow rate, density and melting point, so you can shortlist by process before you request a sample.

Contents

What EMA and EBA Are — and How They Differ

Both resins are made by copolymerising ethylene with an acrylate monomer. The polyethylene backbone gives toughness, chemical resistance and processability on conventional PE equipment. The acrylate units disrupt crystallinity and add polarity, which is what makes the resin softer, more flexible and more willing to bond to polar surfaces than plain LDPE or LLDPE.

The practical difference is the comonomer:

  • EMA uses methyl acrylate. In the SK LOTRYL range these are the grades whose code carries an "MA" — for example 18MA02, 24MA02 and 29MA03.
  • EBA uses butyl acrylate. In the same range these are the "BA" grades — 30BA02, 35BA40, 35BA320 and the 28BA high-flow grades.

A longer acrylate side chain generally gives a softer, more flexible polymer at equivalent comonomer content. In the published LOTRYL data, the BA grades are conspicuously soft: 35BA320T is listed with a tensile strength of 1.3 MPa and elongation at break of 110%, while 30BA02 — a low-flow BA grade — is listed at 6 MPa tensile and 850% elongation. The MA grades span a wider mechanical range, from the low-flow 24MA005 at 17 MPa tensile and 750% elongation to the higher-flow 29MA03 at 6 MPa and 900%.

One caution up front: several pages in our catalogue carry the joint title "EMA / EBA Copolymer Pellets" because that is how the material was described in the source documentation. Where the grade code contains "MA" or "BA", that code is the reliable indicator of which copolymer you are looking at. If the code does not tell you — as with the Exxtra TC and EN numbers — ask for the comonomer in writing before you specify.

Melt Flow Rate Is the First Filter, Not the Last

The single most useful number for shortlisting is melt flow rate (MFR), because it tells you whether the grade fits your equipment at all. The LOTRYL pages state their MFR condition as 190 °C / 2.16 kg; keep the test condition attached to the number, since a flow rate without a condition is not comparable.

Across the 25 grades listed here, MFR runs from 0.5 g/10 min at the low end (24MA005) to 700 g/10 min at the high end (28BA700T). That is a spread of more than three orders of magnitude, and it splits the range into three practical groups:

GroupMFR (190 °C / 2.16 kg)Representative gradesTypical fit
Low flow0.5–324MA005, 24MA02, 29MA03, 30BA02, TC110Film, blown film, extrusion where melt strength matters
Mid flow5–820MA08, 28MA07, 24MA07T, TC121, TC220Extrusion coating, general compounding
High flow40–70035BA40, 28BA175, 35BA320, 28BA700T, EN33331Hot melt adhesive, masterbatch carrier, high-speed coating

Do not stop at MFR, though. Two grades with identical flow can behave very differently in melting point and stiffness. 24MA02 and 24MA02T are both listed at MFR 2, but their melting points are 68 °C and 95 °C respectively. If your process runs near the softening point, that difference decides whether the grade works.

The LOTRYL "MA" Grades (EMA)

The table below reproduces the published values on our product pages. Density is in g/cm³, melting point in °C, tensile in MPa, elongation in %, flexural modulus in MPa. A dash means the field is not stated in the source data — we do not fill it in.

GradeMFRDensityMeltingVicatTensileElongationFlexural
18MA0220.9483531370050
20MA0880.947646980020
24MA0220.9468491280018
24MA02T20.9395401280017
24MA0050.50.9572451775018
24MA07T70.959749550036
28MA0770.946540790010
29MA0330.946140690010
29MA03T30.9492401090012

Two patterns are worth noting. First, the grades ending in "T" consistently show a higher melting point than their non-T neighbours with the same flow — 24MA02 vs 24MA02T (68 vs 95 °C), 29MA03 vs 29MA03T (61 vs 92 °C). If you need heat resistance without giving up flow, the T variants are the ones to screen. Second, 24MA005 is the only sub-1 MFR grade in the EMA set and carries the highest listed tensile value (17 MPa), which makes it a candidate where melt strength and tear resistance matter more than line speed.

The LOTRYL "BA" Grades (EBA)

The BA side of the range covers both very low-flow film grades and some of the highest-flow resins in the whole catalogue. Values below are as published.

GradeMFRDensityMeltingVicatTensileElongationFlexural
28BA1751750.949740——10
28BA175T1750.944040———
28BA700T7000.949440——10
30BA0220.94754168509
35BA40400.946640260010
35BA3203200.946540220010
35BA320T3200.9490401.311010

The high-flow end is where EBA earns its keep. 28BA700T at MFR 700 and 35BA320 at 320 are in hot-melt and high-speed coating territory; their low elongation figures (200% and below) reflect that they are not chosen for stretch. At the other end, 30BA02 at MFR 2 combines 850% elongation with a 75 °C melting point, which suits flexible film and sheet. We have left tensile and elongation blank for the 28BA grades where the source data did not state them — request the TDS if those values are decisive for your application.

The Exxtra TC and EN Grades

The ExxonMobil Exxtra entries in our catalogue are titled EMA / EBA Copolymer Pellets, but the grade numbers do not encode the comonomer the way LOTRYL codes do. Treat the comonomer as unconfirmed until you see the TDS. The published physical data is as follows.

GradeMFRDensityMelting
TC11020.94380
TC11120.94380
TC11420.94781
TC120EXCO60.94379
TC12160.94479
TC22050.94472.8
TC22150.94473.3
EN333313300.92361.7
EN33901—0.9262.2

The TC series clusters tightly at MFR 2–6 with melting points of 73–81 °C — a convenient set for screening low-to-mid flow applications where you want similar process behaviour across grades. EN33331 is the outlier: MFR 330, density 0.923 and a melting point of 61.7 °C. EN33901 has no MFR stated in our data, so it cannot be shortlisted on flow until you ask for it.

Choosing by Process

  • Blown or cast film. Start at low flow: 24MA005 (0.5), 24MA02 (2), 30BA02 (2). These give melt strength; 30BA02's 850% elongation suits flexible film.
  • Heat-resistant film or sheet. Screen the "T" versions — 24MA02T (melting 95 °C), 29MA03T (92 °C), 35BA320T (90 °C) — where the base grade melts in the 60s.
  • Extrusion coating. Mid flow is the usual starting point: 20MA08 (8), 28MA07 (7), TC121 (6), TC220 (5).
  • Hot melt adhesive or masterbatch carrier. Go high flow: 35BA40 (40), 28BA175 (175), 35BA320 (320), 28BA700T (700), EN33331 (330).
  • Maximum softness. The BA grades are the softer family in the published data; 35BA320T lists 1.3 MPa tensile, versus 17 MPa for the stiffest EMA grade 24MA005.

Where your application needs adhesion to aluminium foil, paper or PA rather than flexibility alone, EAA and EMAA are a different family — acid copolymers rather than acrylate esters. We cover that separately in EAA and EMAA Adhesive Resins: The Quiet Hero of Multilayer Packaging. If the bond is to a polar substrate, read that guide before you lock an EMA/EBA grade.

What to Confirm Before You Place an RFQ

  1. Comonomer in writing. For LOTRYL, read MA vs BA in the code. For TC and EN grades, ask explicitly.
  2. MFR with its test condition. Our LOTRYL pages state 190 °C / 2.16 kg. Confirm the same condition on any replacement grade.
  3. Melting point and Vicat if the part sees heat in service or in a downstream process.
  4. Which fields are actually stated. Several high-flow grades have no tensile or elongation value in the source; do not assume they match a neighbouring grade.
  5. Batch documentation. Ask for the grade TDS and batch COA; see How to Read a Third-Party Polymer Test Report for how to check what a document actually covers.

FAQ

Are EMA and EBA the same as EAA? No. EMA and EBA are acrylate esters; EAA is ethylene-acrylic acid. The acid family is the one normally selected for foil and paper adhesion. See the EAA/EMAA guide linked above.

Which is softer, EMA or EBA? In the published LOTRYL data, the BA grades reach lower tensile values (down to 1.3 MPa for 35BA320T) than the MA grades, which is consistent with a softer material. Softer is not automatically better — check elongation and melting point against your process.

Can I run these on LDPE equipment? The MFR range overlaps LDPE processing, but the melting points and melt strength differ grade by grade. Start from the MFR group table above and confirm with the TDS.

Why are some values blank in your tables? Because the source document did not state them. We leave the field empty rather than estimating. Ask us for the specific TDS if you need it.

Browse the grades behind this guide: 18MA02, 24MA02, 30BA02, 28BA700T, TC110.