Quick answer. On a thin-wall PP part, a sink mark is almost never fixed by changing the resin first. It means a thick region — a rib, boss or gate land — stayed molten after the surface skin froze, and pulled that skin inward as it shrank. Check rib thickness against the local wall first (keep it at or below roughly half the wall), then gate location and packing, and only then look at the grade’s shrinkage and flow. POE changes stiffness and flow, but it does not cancel a thick section.
Sink marks are the most common cosmetic rejection on thin-wall injection-moulded polypropylene parts, and the most commonly misdiagnosed. The usual response is to change material or add more packing pressure. Sometimes that works. More often the thick region is simply too thick for the surrounding wall, and no grade change will make the depression disappear.
What a sink mark actually is
A moulded part cools from the outside in. The surface skin freezes first; the core stays molten longer and continues to contract. Where the section is uniform, that contraction shows up as the part getting slightly smaller overall — which is what mould shrink allowance is for. Where a region is thicker than its surroundings, the extra contraction has to go somewhere visible, and the frozen skin is pulled inward. That is the depression you see.
The scale is larger than most people expect. Unfilled PP is commonly cited at 1.5–2% linear shrinkage, roughly 4–6% by volume. Even Borealis’s data sheet for its HE125MO thin-wall PP grade gives 1–2% and explicitly says it depends on wall thickness and moulding parameters. A published design guide illustrates the effect with rib-to-wall ratios: at 0.4× the wall the predicted sink is about 2 µm, at 0.5× about 6 µm, but at 0.8× about 38 µm and at 1.0× about 62 µm — at which point the mark is obvious. Treat those numbers as an illustration of the trend, not as a specification for your part.
Key variables, in the order that matters
- Local thickness ratio, not nominal wall. Rib bases, boss roots and gate lands are the usual offenders. Common guidance is to keep ribs at 0.5–0.6× the local wall (0.4–0.5× on a cosmetic face), rib height at or below 3× wall, rib spacing at least 2× wall, and internal corner radius at least 0.5× wall.
- Gate location and packing path. A rib far from the gate freezes before holding pressure reaches it. Moving a gate or adding a local gate often beats raising holding pressure, which just pumps more material into sections that are already fed.
- Grade shrinkage and flow length. PP grades differ; unfilled PP is usually quoted at 1.5–2.5% and glass-filled at 0.5–1.0% but directionally. Thin walls need flow — PP parts are commonly designed around 1–3 mm walls, and going thinner sharply raises flow resistance.
- Modifier level and density. POE improves impact but lowers tensile and flexural modulus; published industry data also suggests melt flow stops climbing much beyond about 15 phr. So adding POE to “help flow” has a ceiling, and adding it for impact can soften the part. See how POE density affects stiffness retention for the density side of that trade-off.
- Process window. For one thin-wall PP grade, the supplier sheet lists melt 220–260 °C, mould 20–40 °C and holding pressure 200–500 bar. That is illustrative for one grade, not a recipe — but if your settings sit outside a supplier’s stated window, the grade is the first thing to check.
Common fixes and what they cost
“Turn up holding pressure and time.” Cheap and often the right first move — but it only helps regions the packing front can still reach. Beyond that it raises residual stress and can cause ejection distortion or flash.
“Switch to a lower-shrinkage grade.” Legitimate when the whole part is oversized or warped, less useful when only one rib is marked. A grade change affects cost, impact and cycle time at once, and it cannot remove a thick section.
“Add more POE to make it flow and stay tough.” This trades stiffness for impact, and the flow benefit flattens out. If the part feels soft afterwards, that is the trade showing up — see why a toughened PP part feels too soft. For loading arguments, why “8%” and “25%” both sound right explains why there is no single correct number.
How we work through it
We start with geometry, because that is where the defect is defined: measure the rib or boss against the wall right next to it, not against the nominal wall on the drawing. If the ratio is above roughly half, correct that before touching the material. Then check whether the marked region is fed — gate position and distance matter more than pressure magnitude. Only when geometry and packing are sound do we look at grade shrinkage, flow length and modifier level together.
That last step is where grade selection earns its keep. The grade should match the flow length and the stiffness the part needs — not be asked to compensate for a thick rib.
Reference ranges (with conditions)
| Item | Typical range | Condition / caveat |
|---|---|---|
| Unfilled PP linear shrinkage | 1.5–2.5% | General published ranges; one supplier grade states 1–2%. Verify against your grade’s own TDS. |
| Glass-filled PP shrinkage | 0.5–1.0% | Directional — more along flow than across it. |
| Rib thickness / local wall | 0.5–0.6×; 0.4–0.5× on cosmetic face | Geometry rule; rib height ≤3× wall, spacing ≥2× wall. |
| PP part wall thickness | Commonly 1–3 mm | Flow length and grade determine the real window; published guidance ranges up to ~3.8 mm. |
| Example thin-wall PP processing window | Melt 220–260 °C; mould 20–40 °C; hold 200–500 bar | One supplier grade’s published sheet only. Illustrative, not a setting recommendation. |
| POE loading effect | Modulus falls as loading rises; flow benefit levels off beyond ~15 phr (industry source) | Direction only. No universal “correct” percentage; validate in your own part. |
Grades worth checking, by what they let you do
These are real, published grades on this site. They are grouped by the trade-off they represent — none of them “fixes” sink marks on its own.
- DOW ENGAGE 8400 — density 0.870 g/cm³, MFR 30 g/10 min (190 °C/2.16 kg). A high-flow option when thin walls and long flow paths are the constraint; flow helps filling, not shrinkage control.
- DOW ENGAGE 8450 — density 0.902 g/cm³, MFR 3 g/10 min (190 °C/2.16 kg). The higher-density end of the range, for cases where stiffness retention matters more than maximum flow.
- DOW ENGAGE 8842 — density 0.857 g/cm³, MFR 1 g/10 min (190 °C/2.16 kg). Very low density and low flow; useful as the opposite end of the comparison, not a default for thin-wall fill.
Values above are taken from each grade’s published page on this site. Check the full POE / OBC grade list to compare the rest of the range.
FAQ
Does adding more holding pressure remove sink marks?
It helps only where packing can still reach the region. For a rib that has frozen before the holding phase, pressure cannot get through. Fix the thickness ratio or the gate position first.
What is the half-wall rule?
A rib should be no thicker than about half the wall it sits on — commonly quoted as 0.5–0.6× (0.4–0.5× on a visible face). Above that, the predicted sink depth rises steeply.
Can a different POE grade eliminate sink marks?
No grade removes a thick section. POE affects flow, impact and stiffness; those change how a part fills and how much it contracts overall, but a boss that is the same thickness as the wall will still mark.
Why does one supplier say 1–2% shrinkage and another say 1.5–2.5%?
They are different grades with different test conditions, and shrinkage depends on wall thickness and processing. Use the range on your own grade’s data sheet, not a generic number.
Is a sink mark the same as a void?
Same cause — a thick region contracting after the skin freezes — different symptom. If the surface stays flat and the hollow is internal, it is a void; if the surface pulls inward, it is a sink.