Two POE grades at the same loading can leave a PP compound with visibly different stiffness. The variable doing the work is density — and it is the one most often left out of the substitution conversation, because density is easy to match on paper and hard to match in a part.
The situation
The impact test passes, the part ships, and three weeks later the customer says it feels soft, or a clip no longer holds, or a panel bows under load. The instinct is to reduce POE loading. That fixes the stiffness and re-opens the impact problem — because the real lever was never the percentage, it was which POE went into the percentage.
What density is actually doing
POE density is a proxy for crystallinity and comonomer content. Lower density means more comonomer (typically octene), less crystallinity, a softer elastomer, and better low-temperature impact per percent added. Higher density means less comonomer, more crystallinity, an elastomer that behaves closer to a plastomer: it dilutes the PP matrix less, so modulus holds better, but each percent buys less impact.
That gives the trade in its simplest form:
- Lower density — more impact per percent, more stiffness lost per percent, better low-temperature behaviour, often tackier and harder to handle at high loading.
- Higher density — less impact per percent, less stiffness lost, better flow behaviour in thin sections, closer to the base resin in thermal behaviour.
Comonomer type matters on top of this. Octene-based grades at a given density generally deliver better impact efficiency and elastic recovery than butene-based grades; butene grades are usually the cheaper route where a slightly weaker low-temperature result is acceptable. Two grades at 0.868 are not the same material if one is octene and the other butene.
Where the common practice goes wrong
- Substituting on density and MFR alone. Those two numbers get you into the right family, not to an equivalent. The impact curve has to be re-run.
- Raising density without lowering loading. If you move from 0.868 to 0.885 at the same percentage, you usually lose impact and gain stiffness — then the next trial adds loading back and you are chasing your own tail.
- Chasing stiffness with filler first. Talc buys modulus cheaply, but it also embrittles and raises density; starting with the elastomer choice is usually cheaper than fixing it afterwards.
- Ignoring MFR at the same density. MFR changes dispersion and weld-line behaviour. A 0.5 MFR grade and a 30 MFR grade at the same density are different tools, not different grades of the same tool.
How we approach it
- Write down the stiffness floor first — flexural modulus or a deflection limit on the actual part, not a generic datasheet value.
- Pick the density band from that floor: the higher the floor, the higher the density you can afford.
- Set loading second, inside the band, using a three-point ladder rather than a single trial.
- Only then tune MFR for the process — flow for thin walls, melt strength for extrusion or blow moulding.
- Re-check low-temperature impact at the end. It is the property that quietly disappears when you chase modulus.
Reference bands
Density values below are real grade data from our catalogue. Behaviour descriptions are directional and reflect how these bands are used in practice — they are not test results for your compound.
| Density band (g/cm³) | Behaviour in PP | Typical use |
|---|---|---|
| 0.855–0.862 | Highest impact efficiency, softest, most modulus loss | Low-temperature impact, foam, very tough parts |
| 0.863–0.872 | Balanced: the general-purpose toughening band | Automotive compounds, appliance housings, general moulding |
| 0.873–0.882 | Modulus retained better, impact efficiency drops | Parts with a stiffness floor or thin walls |
| 0.883–0.910 | Plastomer-like: closest to base resin, least toughening per percent | Film, sealing layers, moderate toughening with modulus priority |
Grades to compare
Same ladder, four real grades we stock: Dow ENGAGE 8842 (0.857, MFR 1) at the soft end, Dow ENGAGE 8157 (0.868, MFR 0.5) in the general-purpose band, Dow ENGAGE 7270 (0.880, butene-based) where modulus matters, and Dow ENGAGE 8003 (0.885, MFR 1) at the stiff end.
Cross-brand equivalents at the same density exist — for example SABIC FORTIFY C0570 at 0.868 and SK SOLUMER 851L at 0.857. Treat them as trial candidates, not drop-in replacements, until the impact curve matches.
Density only sets the slope. How far along that slope you travel is the loading decision — covered in POE loading in PP: why “8%” and “25%” both sound right.
FAQ
Does higher density always mean better stiffness retention?
At equal loading and equal comonomer type, yes — that is the direction. It is not a straight line, and it stops being useful once the grade is so plastomer-like that you are barely toughening the PP at all.
Can I hold stiffness by adding filler instead of changing grade?
You can, and many compounds do. But filler raises density, hurts low-temperature impact and adds a dispersion step. Changing the elastomer band is usually the cheaper first move.
Is a 0.868 octene grade equivalent to a 0.868 butene grade?
No. Expect better impact efficiency and elastic recovery from the octene grade, and a lower price from the butene grade. Match the property you need, not the number on the certificate.
How many trials does a density change need?
Three points on the loading ladder at the new density, plus a control at your current formulation. Anything less and you cannot tell grade effect from process noise.