A customer sends you a part that passed at +23 °C, failed at -40 °C, and asks for the "equivalent" of what they were using. Both candidate grades carry epoxy groups, so the swap looks safe on paper. It often is not.
LOTADER AX8900 and ELVALOY PTW sit in the same family - GMA-functionalised ethylene terpolymers used as reactive tougheners and compatibilisers - and they are routinely treated as interchangeable because both are sold on the phrase "epoxy functional". The reactive group is only the part that attaches to the matrix. Everything else in the chain decides whether the part survives the winter test.
This note covers what is actually shared, what differs, and how to choose between them without guessing.
Who this is for
Compounders and buyers formulating against polyamide, polyester or their alloys, where a toughener has to bond to the matrix rather than merely sit in it. If your matrix is polyolefin (PP, PE), start with physical toughener and elastomer selection instead - the reactive mechanism below does not apply the same way.
What the two grades genuinely share
Both are ethylene-based terpolymers carrying methyl methacrylate glycidyl ester (GMA) as a reactive comonomer. During compounding, the epoxy ring opens in situ and reacts with end groups available in polar matrices - carboxyl and hydroxyl end groups in PET, PBT and PA. That in-situ reaction does two things that physical blending cannot: it lowers interfacial tension enough to refine the dispersed rubber phase, and it chemically anchors that phase to the matrix so stress is actually transferred rather than the phase pulling out.
Two boundaries worth stating plainly:
- The end-group chemistry above is well established for polyesters and polyamides. For PC and PPS, the reactive pathways differ (end-group and transesterification routes on PC; different reactive sites on PPS), so treat data generated on PBT or PA as indicative, not transferable.
- We describe the dispersed phase as fine and interfacially bound because that is what reactive compatibilisation is for. The exact domain size in your system is a microscopy question, not a datasheet line.
Where they diverge: MA versus BA
The third comonomer is where the products part company. AX8900 uses methyl acrylate (MA); PTW uses butyl acrylate (BA). Both soften the ethylene backbone, but by different amounts.
A methyl ester side chain is short. It disrupts ethylene crystallinity, yet it does not create much free volume between chains, so segmental mobility stays comparatively limited and the rubber phase keeps some modulus. A butyl side chain carries four carbons: it props the chains further apart, chain segments move easily, and the glass transition of the elastomer drops sharply - PTW is commonly quoted around -55 °C, which is why it stays elastomeric in deep-cold service.
| LOTADER AX8900 | ELVALOY PTW | |
|---|---|---|
| Composition | E - MA - GMA | E - BA - GMA |
| Comonomer that sets flexibility | Methyl acrylate (short side chain) | Butyl acrylate (long side chain) |
| Reported GMA level | ~8% (published grade data) | ~5% class level; the figure of 5.25% circulates in trade literature and is not on a public producer TDS |
| Tg of the elastomer | Higher - stiffer rubber phase | Commonly quoted near -55 °C |
| Melting point | ~65 °C (published grade data) | ~72 °C (trade literature; confirm on current TDS) |
| Melt index | ~6 g/10 min (190 °C / 2.16 kg, published grade data) | ~12 g/10 min (published grade data) |
| Practical tendency | More reactive sites, better stiffness retention | Lower Tg, easier flow, deeper cold performance |
Two numbers in the table are flagged on purpose. Sourcing your figures is not decoration: it is what allows a reader to reproduce your conclusion, and it is the difference between a technical note and a sales sheet. Read the numbers as directions of travel, not as your recipe.
Room-temperature toughening: AX8900 usually has the edge
For ordinary toughening and compatibilisation duty, two effects favour the MA-based grade:
- More reactive sites per unit weight. A higher GMA level means more epoxy available for interface formation, so it generally works harder as a compatibiliser at lower loading.
- Stiffness is preserved better. A shorter side chain leaves the dispersed phase with more modulus, so fracture elongation and impact rise while flexural modulus holds up. For parts that must not go soft - thin-wall housings, snap fits, automotive clips - that balance usually matters more than a higher impact number.
On inherently rigid matrices such as PC, PBT and PPS alloys, this "rigidity retention first" bias is usually what you are buying.
The -40 °C case: two genuinely different routes
Deep-cold impact is where a wrong equivalence becomes a field failure. There are two working routes, and each has a price that is rarely quoted.
Route A - one product, high loading
A BA-based grade near -55 °C Tg is still elastomeric at -40 °C, so a single reactive toughener dosed high can reach extreme low-temperature toughness in one step. Its higher melt index also partially offsets the viscosity rise caused by chain extension and branching during the reactive process.
The price: in binary polyester systems, toughener loadings in this range are reported to cost a large fraction of tensile and flexural strength - literature on PBT/PTW blends puts the loss near half. You are trading stiffness for survive-the-cold, and you should confirm the residual values against your own spec sheet, not against a general claim.
Route B - split the functions
Use a small amount of the high-GMA grade as the chemical anchor at the interface, and carry the bulk of the toughening on a separate, high-flow physical modifier. A typical shape:
- 2-3% of the high-GMA grade, doing phase refinement and interfacial bonding;
- 5-10% of a high-flow elastomer to carry elongation and to bring melt viscosity back down.
The second component is where EBA/EMA chemistry earns its place; our EMA vs EBA grade map compares methyl and butyl acrylate copolymers by melt flow and flexibility, and for polyolefin work see the POE grade map.
The benefit is control: you tune the interface with one variable and the bulk rheology with the other, instead of pushing a single product into a compromise. This matters most on large thin-wall parts, where filling is the binding constraint.
Decision table
| Your binding requirement | Where to start |
|---|---|
| Room-temperature toughening while holding flexural modulus (PC, PBT, PPS alloys) | High-GMA MA-based grade (AX8900 class) |
| -40 °C impact, stiffness secondary | BA-based grade (PTW class) at elevated loading - then verify retained tensile and flexural values |
| -40 °C impact and mould filling on thin walls | Reactive anchor (2-3%) plus high-flow physical modifier (5-10%) |
| Viscosity already tight, chain extension is unwelcome | Prefer the higher-MI grade, or reduce reactive loading and compensate physically |
| Multi-layer film tie layer rather than bulk toughening | Different product set entirely - see tie-layer & compatibilisers, what a tie-layer resin is and tie-layer MFR selection |
| Delamination on an existing film line | Rule out process causes first: delamination troubleshooting |
Grades we currently list in this family: SK LOTADER 4210, SK LOTADER 3430, Dow Bynel 21E787 and Sumitomo Igetabond BF-7L. AX8900 and ELVALOY PTW are both available through us on request - tell us the matrix, the target property and the part geometry, and we will match the route rather than a datasheet.
Before you substitute, five checks
- Confirm the TDS revision. GMA and comonomer levels, MFR and melting point all move between document revisions. Our guide to reading a TDS and COA lists the fields worth verifying first.
- Small-scale trial on your own base resin. Same grade, different supplier lot or recycled content, and the reactive outcome shifts.
- Measure the trade, not just the win. Report impact gain alongside retained tensile and flexural modulus.
- Watch melt viscosity through the whole machine, not only the die. Reactive systems creep in viscosity as residence time increases.
- Check drying and moisture. Hydrolysis competes directly with the reaction you are paying for.
Frequently asked questions
Are AX8900 and ELVALOY PTW interchangeable? No, not one-for-one. They share the GMA epoxy anchor, so both bond to polyester and polyamide matrices, but the MA versus BA backbone changes Tg, melt flow and stiffness retention. Substitution requires a re-trial.
Which one is more reactive? The higher-GMA product generally offers more reaction sites per unit weight, which is why the MA-based grade usually acts as the stronger interface former at low loading.
Which one handles deep cold better? The BA-based chemistry, because its elastomer Tg sits far lower. Commonly quoted around -55 °C, it remains elastomeric at -40 °C service temperatures.
Can I just add more of either to pass a cold test? You usually can reach the impact target, at the cost of stiffness and strength. Reported losses in binary polyester systems are large; verify retained values against your specification.
Why does my melt viscosity rise when I add a reactive toughener? Epoxy end-groups couple and extend chains during residence. Higher-activity grades raise viscosity more; this is the main reason a high-GMA anchor is often paired with a high-flow physical modifier.
Is this chemistry relevant for PP toughening? Not in the same way. PP has no end groups to react with, so POE-based physical toughening is the normal route. See our POE and OBC grades.
Data sourcing and date. Composition and property figures quoted above come from published grade data and widely circulated trade literature, and are marked in the table where the source is weaker. They are directional references, not batch data, and not a formulation. Grades and properties change: confirm every number against the producer's current TDS, and validate any formulation with small-scale trials on your own equipment before committing production.
Trademarks. LOTADER is a trademark of SK Functional Polymer (business acquired from Arkema Functional Polyolefins). ELVALOY is a trademark of Dow Inc. (formerly DuPont). Names appear only to identify commercial grades; this page is independent technical discussion and is not affiliated with or endorsed by either producer.
Last reviewed: November 2026.